{"id":22447,"date":"2026-09-17T14:16:23","date_gmt":"2026-09-17T06:16:23","guid":{"rendered":"https:\/\/nkmceramic.com\/?p=22447"},"modified":"2026-09-17T14:16:23","modified_gmt":"2026-09-17T06:16:23","slug":"rsic-tiegel-fallstudie","status":"publish","type":"post","link":"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/","title":{"rendered":"Problem bei der Verwendung von rekristallisierten Siliciumcarbid-Tiegeln w\u00e4hrend der Quarzh\u00e4rtung: Fallstudie"},"content":{"rendered":"<p>Recrystallized silicon carbide provides excellent thermal stability with chemical corrosion resistance. RSiC crucibles are the ideal choice for high-temperature applications to bring consistent output. Nevertheless, even high-quality RSiC crucibles may face certain problems due to improper design and setup.<\/p>\n<p>In this article, you will find the causes and solutions to those problems through a practical case of RSiC crucible failure.<\/p>\n<div id=\"ez-toc-container\" class=\"ez-toc-v2_0_82_2 counter-hierarchy ez-toc-counter ez-toc-grey ez-toc-container-direction\">\n<div class=\"ez-toc-title-container\">\n<p class=\"ez-toc-title\" style=\"cursor:inherit\">Table of Contents<\/p>\n<span class=\"ez-toc-title-toggle\"><a href=\"#\" class=\"ez-toc-pull-right ez-toc-btn ez-toc-btn-xs ez-toc-btn-default ez-toc-toggle\" aria-label=\"Toggle Table of Content\"><span class=\"ez-toc-js-icon-con\"><span class=\"\"><span class=\"eztoc-hide\" style=\"display:none;\">Toggle<\/span><span class=\"ez-toc-icon-toggle-span\"><svg style=\"fill: #999;color:#999\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\" class=\"list-377408\" width=\"20px\" height=\"20px\" viewBox=\"0 0 24 24\" fill=\"none\"><path d=\"M6 6H4v2h2V6zm14 0H8v2h12V6zM4 11h2v2H4v-2zm16 0H8v2h12v-2zM4 16h2v2H4v-2zm16 0H8v2h12v-2z\" fill=\"currentColor\"><\/path><\/svg><svg style=\"fill: #999;color:#999\" class=\"arrow-unsorted-368013\" xmlns=\"http:\/\/www.w3.org\/2000\/svg\" width=\"10px\" height=\"10px\" viewBox=\"0 0 24 24\" version=\"1.2\" baseProfile=\"tiny\"><path d=\"M18.2 9.3l-6.2-6.3-6.2 6.3c-.2.2-.3.4-.3.7s.1.5.3.7c.2.2.4.3.7.3h11c.3 0 .5-.1.7-.3.2-.2.3-.5.3-.7s-.1-.5-.3-.7zM5.8 14.7l6.2 6.3 6.2-6.3c.2-.2.3-.5.3-.7s-.1-.5-.3-.7c-.2-.2-.4-.3-.7-.3h-11c-.3 0-.5.1-.7.3-.2.2-.3.5-.3.7s.1.5.3.7z\"\/><\/svg><\/span><\/span><\/span><\/a><\/span><\/div>\n<nav><ul class='ez-toc-list ez-toc-list-level-1 ' ><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-1\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#What_is_an_RSiC_Crucible\" >What is an RSiC Crucible?<\/a><ul class='ez-toc-list-level-3' ><li class='ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-2\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Properties_of_RSiC_Crucibles\" >Properties of RSiC Crucibles<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-3\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Key_Industrial_Applications\" >Key Industrial Applications<\/a><\/li><\/ul><\/li><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-4\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Real_Case_RSiC_Crucible_Damage_During_Quartz_Curing\" >Real Case: RSiC Crucible Damage During Quartz Curing<\/a><ul class='ez-toc-list-level-3' ><li class='ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-5\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Operating_Conditions\" >Operating Conditions<\/a><ul class='ez-toc-list-level-4' ><li class='ez-toc-heading-level-4'><a class=\"ez-toc-link ez-toc-heading-6\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Observed_Damage_After_the_First_Run\" >Observed Damage After the First Run<\/a><\/li><\/ul><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-7\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Cause_Analysis_of_Crucible_Issues\" >Cause Analysis of Crucible Issues<\/a><ul class='ez-toc-list-level-4' ><li class='ez-toc-heading-level-4'><a class=\"ez-toc-link ez-toc-heading-8\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Outer_Surface_Blistering_Near_Heating_Elements\" >Outer Surface Blistering Near Heating Elements<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-4'><a class=\"ez-toc-link ez-toc-heading-9\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Crucible_Bottom_and_Sidewall_Separation\" >Crucible Bottom and Sidewall Separation<\/a><\/li><\/ul><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-10\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Practical_Solutions_and_Usage_Optimization_Tips\" >Practical Solutions and Usage Optimization Tips<\/a><ul class='ez-toc-list-level-4' ><li class='ez-toc-heading-level-4'><a class=\"ez-toc-link ez-toc-heading-11\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Adjust_Crucible_Position\" >Adjust Crucible Position<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-4'><a class=\"ez-toc-link ez-toc-heading-12\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Add_Alumina_Spacers\" >Add Alumina Spacers<\/a><\/li><\/ul><\/li><\/ul><\/li><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-13\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Solutions_to_Extend_RSiC_Crucible_Service_Life\" >Solutions to Extend RSiC Crucible Service Life<\/a><ul class='ez-toc-list-level-3' ><li class='ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-14\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Optimize_Thermal_Cycle_Control\" >Optimize Thermal Cycle Control<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-15\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Standardize_Loading_Operation\" >Standardize Loading &amp; Operation<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-16\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Add_Protection_For_Corrosive_Applications\" >Add Protection For Corrosive Applications<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-3'><a class=\"ez-toc-link ez-toc-heading-17\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Establish_Regular_Inspection_And_Maintenance_Routines\" >Establish Regular Inspection And Maintenance Routines<\/a><\/li><\/ul><\/li><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-18\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#FAQs\" >FAQs<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-19\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Conclusion\" >Conclusion<\/a><\/li><li class='ez-toc-page-1 ez-toc-heading-level-2'><a class=\"ez-toc-link ez-toc-heading-20\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/#Reference\" >Reference<\/a><\/li><\/ul><\/nav><\/div>\n\n<h2><span class=\"ez-toc-section\" id=\"What_is_an_RSiC_Crucible\"><\/span><strong><b>What is an RSiC Crucible?<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p>Let\u2019s get a briefly review RSiC before examining the case study.<\/p>\n<p><strong><b>Read More: <\/b><\/strong><a href=\"https:\/\/nkmceramic.com\/what-is-a-ceramic-crucible\/\"><u>What is a Ceramic Crucible?<\/u><\/a><\/p>\n<h3><span class=\"ez-toc-section\" id=\"Properties_of_RSiC_Crucibles\"><\/span><strong><b>Properties of RSiC Crucibles<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>RSiC is a highly pure ceramic that has been made using very high sintering temperatures. The material remains mechanically strong even at 1,600\u2103 or higher temperatures, and also withstands thermal shock and chemical attacks by most molten industrial materials.<\/p>\n<p>These make it ideal for long, continuous high-temperature production runs.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Key_Industrial_Applications\"><\/span><strong><b>Key Industrial Applications<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>RSiC crucibles are normally used in quartz powder lines. They are also extensively used in ceramic sintering and powder metallurgy processes.<\/p>\n<p>Many users upgrade to RSiC from standard SiC for longer service life.<\/p>\n<h2><span class=\"ez-toc-section\" id=\"Real_Case_RSiC_Crucible_Damage_During_Quartz_Curing\"><\/span><strong><b>Real Case: RSiC Crucible Damage During Quartz Curing<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p>We recently supported a client who faced unexpected crucible failure after first use. Their experience illustrates 2 frequent issues you may also face in your operations.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Operating_Conditions\"><\/span><strong><b>Operating Conditions<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>The client tested a new RSiC crucible for quartz powder curing treatment. Their furnace operated at a target temperature of 1,600\u2103 per batch. Heating and cooling rates were set between 2 and 3\u2103 per minute. Peak temperature was held for 2 to 3 hours for each processing cycle.<\/p>\n<h4><span class=\"ez-toc-section\" id=\"Observed_Damage_After_the_First_Run\"><\/span><strong><b>Observed Damage After the First Run<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h4>\n<p>When the client opened the furnace after the weekend run, they found 2\u00a0problems.<\/p>\n<ul>\n<li>The crucible bottom had fully separated from the sidewall structure.<\/li>\n<li>Noticeable blistering appeared on the outer sidewall surface.<\/li>\n<\/ul>\n<p>They had used other types of SiC crucibles for years without similar issues.<\/p>\n<p>The client reached out to investigate potential manufacturing defects. They also wanted to know if specific furnace conditions caused the damage.<\/p>\n<figure id=\"attachment_22449\" aria-describedby=\"caption-attachment-22449\" style=\"width: 1280px\" class=\"wp-caption alignnone\"><img decoding=\"async\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" data-src=\"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\" class=\"size-full wp-image-22449 lazyload\" alt=\"The Client Provided Photos Showing Separation at the Bottom of the Crucible\" width=\"1280\" height=\"720\"><figcaption id=\"caption-attachment-22449\" class=\"wp-caption-text\"><noscript><img decoding=\"async\" class=\"size-full wp-image-22449\" src=\"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\" alt=\"The Client Provided Photos Showing Separation at the Bottom of the Crucible\" width=\"1280\" height=\"720\" srcset=\"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg 1280w, https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible-768x432.jpg 768w, https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible-18x10.jpg 18w\" sizes=\"(max-width: 1280px) 100vw, 1280px\" \/><\/noscript> The Client Provided Photos Showing Separation at the Bottom of the Crucible<\/figcaption><\/figure>\n<h3><span class=\"ez-toc-section\" id=\"Cause_Analysis_of_Crucible_Issues\"><\/span><strong><b>Cause Analysis of Crucible Issues<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>Our technical team reviewed the photos and furnace setup details. We ruled out manufacturing flaws and identified clear operational causes.<\/p>\n<h4><span class=\"ez-toc-section\" id=\"Outer_Surface_Blistering_Near_Heating_Elements\"><\/span><strong><b>Outer Surface Blistering Near Heating Elements<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h4>\n<p>The blisters were concentrated in areas close to silicon molybdenum heating rods.<\/p>\n<p>Silicon molybdenum rods generate intense, highly localized heat during operation. When a crucible sits too near these rods, surface temperatures rise unevenly. This localized overheating triggers blister formation on the crucible exterior.<\/p>\n<p>It is noticed that such blistering does not influence their structural integrity. The crucible is still functional, but blistering can shorten its overall service life.<\/p>\n<h4><span class=\"ez-toc-section\" id=\"Crucible_Bottom_and_Sidewall_Separation\"><\/span><strong><b>Crucible Bottom and Sidewall Separation<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h4>\n<p>First, it should be clarified that high-quality RSiC crucibles are integrally formed, not assembled from parts. They are sintered as a single piece, with no bonded seam between base and sidewall. So separation is not caused by weak adhesive or poor joint manufacturing.<\/p>\n<p>The actual cause is uneven thermal expansion across the crucible body. The crucible bottom was in full, tight contact with the furnace base plate. This tight contact trapped heat and slowed dissipation from the bottom surface.<\/p>\n<p>The sidewall, by contrast, heated and cooled at a very different rate. The resulting thermal stress caused the bottom to pull away from the sidewall. This specific failure mode was a first observation for our technical team.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Practical_Solutions_and_Usage_Optimization_Tips\"><\/span><strong><b>Practical Solutions and Usage Optimization Tips<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>Based on our analysis, we recommended targeted fixes for the client.<\/p>\n<h4><span class=\"ez-toc-section\" id=\"Adjust_Crucible_Position\"><\/span><strong><b>Adjust Crucible Position<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h4>\n<p>The simplest fix for surface blistering is to reposition your crucible.<\/p>\n<p>Move it farther away from the furnace\u2019s silicon molybdenum heating rods. This reduces localized overheating and prevents blister formation.<\/p>\n<p>If furnace space is limited, you can add a lightweight heat shield instead.<\/p>\n<h4><span class=\"ez-toc-section\" id=\"Add_Alumina_Spacers\"><\/span><strong><b>Add Alumina Spacers<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h4>\n<p>To fix uneven heat dissipation at the base, add small support spacers.<\/p>\n<p>For example, use three corundum (alumina) spacers, each about 30mm in diameter. Place them evenly under the crucible to create a narrow air gap.<\/p>\n<p>This gap allows heat to escape freely from the entire bottom surface. Even heat distribution eliminates the thermal stress that causes separation.<\/p>\n<p>The client tested this fix in their next run without further damage reported.<\/p>\n<h2><span class=\"ez-toc-section\" id=\"Solutions_to_Extend_RSiC_Crucible_Service_Life\"><\/span><strong><b>Solutions to Extend RSiC Crucible Service Life<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p>Besides these 2 problems, most of the failure patterns have targeted, field-verified solutions. You can implement these measures in your production line with minimal extra cost.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Optimize_Thermal_Cycle_Control\"><\/span><strong><b>Optimize Thermal Cycle Control<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>Follow a reasonable staged heating curve for cold or brand-new crucibles.<\/p>\n<p>Below 800\u2103, keep the heating rate at 100-120\u2103 per hour.<\/p>\n<p>Between 800\u2103 and 1,400\u2103, you can increase the rate to 150-200\u2103 per hour.<\/p>\n<p>Slow down again above 1,400\u2103.<\/p>\n<p>For cooling, let the crucible cool down with the furnace above 1,000\u2103. Never use forced air cooling or water quenching on hot crucibles.<sup>[1]<\/sup><\/p>\n<h3><span class=\"ez-toc-section\" id=\"Standardize_Loading_Operation\"><\/span><strong><b>Standardize Loading &amp; Operation<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>Preheat solid raw materials before adding them to a hot crucible. Use dedicated tools to lower materials gently.<\/p>\n<p>Do not drop heavy charge from a height, as this causes impact damage and hidden microcracks.<\/p>\n<p>Keep charge volume below 80% of the crucible inner height to prevent overflow.<\/p>\n<p>Distribute heavy materials evenly across the bottom to avoid local stress concentration.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Add_Protection_For_Corrosive_Applications\"><\/span><strong><b>Add Protection For Corrosive Applications<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>For processes with fluoride or alkaline materials, apply a high-purity boron nitride coating on the inner wall. The coating creates a dense isolation layer between the melt and the SiC substrate.<\/p>\n<p>For highly corrosive conditions, you can also use a matching ceramic liner to protect the RSiC crucible body.<\/p>\n<h3><span class=\"ez-toc-section\" id=\"Establish_Regular_Inspection_And_Maintenance_Routines\"><\/span><strong><b>Establish Regular Inspection And Maintenance Routines<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h3>\n<p>Inspect the crucible for surface cracks, corrosion spots, and deformation before each production run. Measure wall thickness at 3-4 key points every month to track wear rate.<sup>[2]<\/sup><\/p>\n<p>Store unused crucibles in a dry, ventilated area. Dry damp crucibles slowly at 100-200\u2103 for 4\u20136 hours before use.<sup>[1]<\/sup><\/p>\n<p>Use soft lifting clamps for handling to avoid edge chipping.<\/p>\n<h2><span class=\"ez-toc-section\" id=\"FAQs\"><\/span><strong><b>FAQ<\/b><\/strong><strong><b>s<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p><strong><b>Are recrystallized silicon carbide crucibles made as one single piece? <\/b><\/strong><\/p>\n<p>Yes. They are not glued or bonded from separate base and sidewall components.<\/p>\n<p><strong><b>Will surface blistering make my RSiC crucible unsafe to operate?<\/b><\/strong><\/p>\n<p>Surface blistering from localized heat does not damage internal structure. It is safe for continued use but may reduce long-term service life.<\/p>\n<p><strong><b>What is the maximum safe operating temperature for an RSiC crucible?<\/b><\/strong><\/p>\n<p>Most standard RSiC crucibles perform reliably up to 1,650\u2103 in air environments. Always refer to your product specification for exact temperature limits.<\/p>\n<p><strong><b>Can I use any hard material as a spacer under my SiC crucible?<\/b><\/strong><\/p>\n<p>No. Only use high-temperature materials like alumina (corundum) or SiC. Lower-grade materials may melt, react, or contaminate your process at high temperatures.<\/p>\n<p><strong><b>How can I tell if crucible damage is a manufacturing defect?<\/b><\/strong><\/p>\n<p>Manufacturing defects typically appear as pre-existing cracks or flaws before first use. Damage after heating cycles almost always links to operating conditions.<\/p>\n<p><strong><b>Can I repair an RSiC crucible that has separated at the bottom?<\/b><\/strong><\/p>\n<p>Bottom separation is structural damage that cannot reliably repaired. Replace the crucible and adjust your furnace setup to prevent future issues.<\/p>\n<h2><span class=\"ez-toc-section\" id=\"Conclusion\"><\/span><strong><b>Conclusion<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p>Most unexpected failures result from setup choices, not manufacturing defects. The case we shared shows how small adjustments can prevent costly production downtime.<\/p>\n<p>If you face challenges with your RSiC crucibles, <a href=\"https:\/\/nkmceramic.com\/\"><u>Newthink <\/u><\/a>technical team can assist you. We dedicate to silicon carbide ceramics since 2011, providing tailored guidance to match your specific furnace and process requirements. <a href=\"https:\/\/nkmceramic.com\/contact-us\/\"><u>Contact us<\/u><\/a>\u00a0for more info\u00a0about customized <a href=\"https:\/\/nkmceramic.com\/silicon-carbide-crucible\/\"><u>RSiC crucibles<\/u><\/a>\u00a0and their maintenance.<\/p>\n<p>Thanks for your reading. Hope this article will be helpful.<\/p>\n<h2><span class=\"ez-toc-section\" id=\"Reference\"><\/span><strong><b>Reference<\/b><\/strong><span class=\"ez-toc-section-end\"><\/span><\/h2>\n<p>[1] <a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S0022024818301763\"><u>Dropka, N., Buchovska, I., Herrmann-Geppert, I., Klimm, D., Kiessling, F. M., &amp; Degenhardt, U. (2018). Towards graphite-free hot zone for directional solidification of silicon.\u00a0<\/u><em><u><i>Journal of Crystal Growth<\/i><\/u><\/em><u>,\u00a0<\/u><em><u><i>492<\/i><\/u><\/em><u>, 18-23.<\/u><\/a><\/p>\n<p>[2] <a href=\"https:\/\/www.jstage.jst.go.jp\/article\/jcersj2\/119\/1387\/119_1387_218\/_article\/-char\/ja\/\"><u>Tanaka, H. (2011). Silicon carbide powder and sintered materials.\u00a0<\/u><em><u><i>Journal of the ceramic society of Japan<\/i><\/u><\/em><u>,\u00a0<\/u><em><u><i>119<\/i><\/u><\/em><u>(1387), 218-233.<\/u><\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>Recrystallized silicon carbide provides excellent thermal stability with chemical corrosion resistance. RSiC crucibles are the ideal choice for high-temperature applications to bring consistent output. Nevertheless, even high-quality RSiC crucibles may face certain problems due to improper design and setup. In this article, you will find the causes and solutions to [&hellip;]<\/p>\n","protected":false},"author":3,"featured_media":22449,"comment_status":"closed","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"disabled","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"default","adv-header-id-meta":"","stick-header-meta":"default","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[1],"tags":[],"class_list":["post-22447","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-blog"],"acf":[],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.1 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study - Newthink Advanced Ceramics<\/title>\n<meta name=\"description\" content=\"Discover why RSiC crucibles fail during quartz curing and how to prevent it. Learn real-world causes, furnace fixes, and tips to extend crucible life.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/\" \/>\n<meta property=\"og:locale\" content=\"de_DE\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study - Newthink Advanced Ceramics\" \/>\n<meta property=\"og:description\" content=\"Discover why RSiC crucibles fail during quartz curing and how to prevent it. Learn real-world causes, furnace fixes, and tips to extend crucible life.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/\" \/>\n<meta property=\"og:site_name\" content=\"Newthink Advanced Ceramics\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/siliconcarbideo\" \/>\n<meta property=\"article:published_time\" content=\"2026-09-17T06:16:23+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\" \/>\n\t<meta property=\"og:image:width\" content=\"1280\" \/>\n\t<meta property=\"og:image:height\" content=\"720\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/jpeg\" \/>\n<meta name=\"author\" content=\"Megan\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Verfasst von\" \/>\n\t<meta name=\"twitter:data1\" content=\"Megan\" \/>\n\t<meta name=\"twitter:label2\" content=\"Gesch\u00e4tzte Lesezeit\" \/>\n\t<meta name=\"twitter:data2\" content=\"7\u00a0Minuten\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/\"},\"author\":{\"name\":\"Megan\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#\\\/schema\\\/person\\\/52ace12691a4a35d94ce801e5ed13362\"},\"headline\":\"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study\",\"datePublished\":\"2026-09-17T06:16:23+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/\"},\"wordCount\":1294,\"publisher\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2026\\\/09\\\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\",\"articleSection\":[\"Blog\"],\"inLanguage\":\"de\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/\",\"url\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/\",\"name\":\"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study - Newthink Advanced Ceramics\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2026\\\/09\\\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\",\"datePublished\":\"2026-09-17T06:16:23+00:00\",\"description\":\"Discover why RSiC crucibles fail during quartz curing and how to prevent it. Learn real-world causes, furnace fixes, and tips to extend crucible life.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#breadcrumb\"},\"inLanguage\":\"de\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#primaryimage\",\"url\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2026\\\/09\\\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\",\"contentUrl\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2026\\\/09\\\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg\",\"width\":1280,\"height\":720,\"caption\":\"The Client Provided Photos Showing Separation at the Bottom of the Crucible\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/rsic-crucible-case-study\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/nkmceramic.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#website\",\"url\":\"https:\\\/\\\/nkmceramic.com\\\/\",\"name\":\"Newthink\",\"description\":\"Advanced Technical Ceramics for Refractories and Demanding Industries\",\"publisher\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/nkmceramic.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"de\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#organization\",\"name\":\"Newthink\",\"url\":\"https:\\\/\\\/nkmceramic.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2025\\\/07\\\/Header-Logo.png\",\"contentUrl\":\"https:\\\/\\\/nkmceramic.com\\\/wp-content\\\/uploads\\\/2025\\\/07\\\/Header-Logo.png\",\"width\":180,\"height\":60,\"caption\":\"Newthink\"},\"image\":{\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/siliconcarbideo\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/nkmceramic.com\\\/#\\\/schema\\\/person\\\/52ace12691a4a35d94ce801e5ed13362\",\"name\":\"Megan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g\",\"caption\":\"Megan\"},\"url\":\"https:\\\/\\\/nkmceramic.com\\\/de\\\/author\\\/megan\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"Problem bei der Verwendung von rekristallisierten Siliciumcarbid-Tiegeln w\u00e4hrend der Quarzh\u00e4rtung: Fallstudie \u2013 Newthink Advanced Ceramics","description":"Erfahren Sie, warum RSiC-Tiegel beim Aush\u00e4rten von Quarz versagen und wie Sie dies verhindern k\u00f6nnen. Lernen Sie die Ursachen in der Praxis kennen, erfahren Sie, wie Sie Ofenreparaturen durchf\u00fchren und erhalten Sie Tipps zur Verl\u00e4ngerung der Tiegellebensdauer.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/","og_locale":"de_DE","og_type":"article","og_title":"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study - Newthink Advanced Ceramics","og_description":"Discover why RSiC crucibles fail during quartz curing and how to prevent it. Learn real-world causes, furnace fixes, and tips to extend crucible life.","og_url":"https:\/\/nkmceramic.com\/de\/rsic-tiegel-fallstudie\/","og_site_name":"Newthink Advanced Ceramics","article_publisher":"https:\/\/www.facebook.com\/siliconcarbideo","article_published_time":"2026-09-17T06:16:23+00:00","og_image":[{"width":1280,"height":720,"url":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg","type":"image\/jpeg"}],"author":"Megan","twitter_card":"summary_large_image","twitter_misc":{"Verfasst von":"Megan","Gesch\u00e4tzte Lesezeit":"7\u00a0Minuten"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#article","isPartOf":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/"},"author":{"name":"Megan","@id":"https:\/\/nkmceramic.com\/#\/schema\/person\/52ace12691a4a35d94ce801e5ed13362"},"headline":"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study","datePublished":"2026-09-17T06:16:23+00:00","mainEntityOfPage":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/"},"wordCount":1294,"publisher":{"@id":"https:\/\/nkmceramic.com\/#organization"},"image":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#primaryimage"},"thumbnailUrl":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg","articleSection":["Blog"],"inLanguage":"de"},{"@type":"WebPage","@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/","url":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/","name":"Problem bei der Verwendung von rekristallisierten Siliciumcarbid-Tiegeln w\u00e4hrend der Quarzh\u00e4rtung: Fallstudie \u2013 Newthink Advanced Ceramics","isPartOf":{"@id":"https:\/\/nkmceramic.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#primaryimage"},"image":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#primaryimage"},"thumbnailUrl":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg","datePublished":"2026-09-17T06:16:23+00:00","description":"Erfahren Sie, warum RSiC-Tiegel beim Aush\u00e4rten von Quarz versagen und wie Sie dies verhindern k\u00f6nnen. Lernen Sie die Ursachen in der Praxis kennen, erfahren Sie, wie Sie Ofenreparaturen durchf\u00fchren und erhalten Sie Tipps zur Verl\u00e4ngerung der Tiegellebensdauer.","breadcrumb":{"@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#breadcrumb"},"inLanguage":"de","potentialAction":[{"@type":"ReadAction","target":["https:\/\/nkmceramic.com\/rsic-crucible-case-study\/"]}]},{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#primaryimage","url":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg","contentUrl":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2026\/09\/1-The-Client-Provided-Photos-Showing-Separation-at-the-Bottom-of-the-Crucible.jpg","width":1280,"height":720,"caption":"The Client Provided Photos Showing Separation at the Bottom of the Crucible"},{"@type":"BreadcrumbList","@id":"https:\/\/nkmceramic.com\/rsic-crucible-case-study\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/nkmceramic.com\/"},{"@type":"ListItem","position":2,"name":"Recrystallized Silicon Carbide Crucible Usage Problem During Quartz Curing:\u00a0Case Study"}]},{"@type":"WebSite","@id":"https:\/\/nkmceramic.com\/#website","url":"https:\/\/nkmceramic.com\/","name":"Newthink","description":"Hochleistungskeramik f\u00fcr feuerfeste Materialien und anspruchsvolle Industrien","publisher":{"@id":"https:\/\/nkmceramic.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/nkmceramic.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"de"},{"@type":"Organization","@id":"https:\/\/nkmceramic.com\/#organization","name":"Newthink","url":"https:\/\/nkmceramic.com\/","logo":{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/nkmceramic.com\/#\/schema\/logo\/image\/","url":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2025\/07\/Header-Logo.png","contentUrl":"https:\/\/nkmceramic.com\/wp-content\/uploads\/2025\/07\/Header-Logo.png","width":180,"height":60,"caption":"Newthink"},"image":{"@id":"https:\/\/nkmceramic.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/siliconcarbideo"]},{"@type":"Person","@id":"https:\/\/nkmceramic.com\/#\/schema\/person\/52ace12691a4a35d94ce801e5ed13362","name":"Megan","image":{"@type":"ImageObject","inLanguage":"de","@id":"https:\/\/secure.gravatar.com\/avatar\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/0a03651a0be7373eda3e9f3e1a31db209654fa157d1f650b24b2e495fc7bb5bd?s=96&d=mm&r=g","caption":"Megan"},"url":"https:\/\/nkmceramic.com\/de\/author\/megan\/"}]}},"_links":{"self":[{"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/posts\/22447","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/users\/3"}],"replies":[{"embeddable":true,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/comments?post=22447"}],"version-history":[{"count":1,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/posts\/22447\/revisions"}],"predecessor-version":[{"id":22450,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/posts\/22447\/revisions\/22450"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/media\/22449"}],"wp:attachment":[{"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/media?parent=22447"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/categories?post=22447"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/nkmceramic.com\/de\/wp-json\/wp\/v2\/tags?post=22447"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}